An iron-carbon alloy initially containing 0.275 wt% C is exposed to an oxygen-rich and virtually carbon-free atmosphere at 1110°C. Under the
Question
An iron-carbon alloy initially containing 0.275 wt% C is exposed to an oxygen-rich and virtually carbon-free atmosphere at 1110°C. Under these circumstances the carbon diffuses from the alloy and reacts at the surface with the oxygen in the atmosphere; that is, the carbon concentration at the surface position is maintained essentially at 0.0 wt% C. At what position will the carbon concentration be 0.206 wt% after a 5 h treatment? The value of D at 1110°C is 5.6 × 10-10 m2/s.
in progress
0
Physics
5 years
2021-08-14T20:39:09+00:00
2021-08-14T20:39:09+00:00 1 Answers
122 views
1
Answers ( )
Answer:
5.12 mm
Explanation:
Let’s convert the time taken from hours to seconds
t = 5 h
t =
t = 18000 s
The relation expressing the concentration, position and time together is given by the formula:
where:
D = diffusion coefficient =
t = time = 18000 s
Replacing the value into the previous formula; we have:
0.2509 = 1 – erf (157.85 x)
erf (157.85 x) = 1 – 0.2509
erf (157.85 x) = 0.7491
So, Let’s assume the value of z to be 157.485x ; we have:
z = 157.485 x —————— Equation (1)
We obtain the value of Z corresponding to erf (Z) = 0.7491 from the Table 5.1 , ‘Table of Error Function Values’
– 0.001895 = (0.75 – z ) 0.0334
– 0.001895 = 0.02505 – 0.0334 z
0.0334 z = 0.02505 + 0.001895
0.0334 z = 0.026945
z =
z = 0.806737
Substituting 0.806737 for z in equation (1)
0.806737 = 157.485 x
x =
x = 0.00512 m to mm; we have
x = 5.12 mm
Thus, the position at which the carbon concentration is 0.206 wt% after a 5 h treatment = 5.12 mm